Influence of Surface Finish on Copper Corrosion in Propylene Glycol-Based Direct-to-Chip Coolants for Data Centers
Dynalene · Carter Prokesch, Sreya Dutta et al.
A Dynalene SEMI-THERM 42 presentation links copper surface roughness (Ra 0.026 to 2.554 µm) to corrosion and BTA film formation in a 25% propylene glycol coolant; 600 to 1500 grit passivates best.
On this page
Overview
The presentation summarizes work by Carter Prokesch, Sreya Dutta and Satish Mohapatra (Dynalene Inc.) at SEMI-THERM 42. It addresses how surface finish affects corrosion of copper cold plates in propylene glycol (PG) based coolant for direct-to-chip (DTC) liquid cooling in data centres.
In the experiments a coolant with 25% glycol, benzotriazole (BTA) and phosphate inhibitor was prepared, and CDA 110 copper coupons were roughened or polished with 60, 240, 600, 1500 and about 8000 grit. Average Ra was 0.026 µm for mirror, 0.220 µm for P1500, 0.138 µm for P600, 0.591 µm for P240 and 2.554 µm for P60. Tests were immersion at 50 °C for 100 h and at 60 °C for 500 h, a heat rejecting condition at 65 °C for 168 h, and electrochemical (potentiodynamic) measurements; inhibitor film was examined by SEM-EDS.
In immersion tests surface nitrogen (the BTA indicator) stayed around 0.96% to 1.80% with no clear dependence on finish. Under the heat rejecting condition (168 h, 65 °C) nitrogen was 18.90% at 600 grit and 9.93% at 1500 grit, against 1.02% to 2.30% at 60, 240 and 8000 grit.
Conclusions: the inhibited coolant markedly improves copper corrosion resistance compared with the uninhibited coolant; scatter in the data stems from the difficulty of polishing cylindrical coupons and non-uniform passivation; heat rejecting copper forms nitrogen-rich lamellar passivating layers between 600 and 1500 grit; high roughness makes inhibitor coverage uncertain while finishes smoother than 1500 grit give too few adhesion points; contaminants complicate passivation, with chloride interfering with nitrogen coverage.
Key points
- Coolant: 25% propylene glycol with BTA and phosphate inhibitors; material CDA 110 copper.
- Average Ra: mirror 0.026, P1500 0.220, P600 0.138, P240 0.591, P60 2.554 µm.
- Tests: immersion 100 h at 50 °C and 500 h at 60 °C; heat rejecting 168 h at 65 °C; electrochemical.
- Nitrogen under heat rejecting condition: 600 grit 18.90%; 1500 grit 9.93%; 8000 grit 1.02%.
- In immersion nitrogen stays about 0.96% to 1.80%.
- Inhibited coolant markedly improves copper corrosion resistance over uninhibited coolant.
- Nitrogen-rich lamellar passivating layers form between 600 and 1500 grit.
- Surfaces smoother than 1500 grit give too few adhesion points for the inhibitor.
- Contaminants such as chloride interfere with BTA coverage.
Using it in design
- Define cold plate copper surface finish as an Ra range in the specification; the study points to 600 to 1500 grit (Ra about 0.14 to 0.22 µm) as the best passivation region.
- Have the manufacturer confirm inhibitor film formation on very rough (P60) or very smooth (about 8000 grit) surfaces.
- Limit contaminants such as chloride and sulfate in the TCS coolant and specify flushing and water quality before commissioning.
- Monitor BTA and phosphate inhibitor concentration in PG25 coolant during operation and request conformity to the coolant supplier's test protocol.
- The work is laboratory scale; the plate maker and coolant supplier should validate jointly under site conditions.
Who should read it
Engineers and chemists selecting direct-to-chip coolants and specifying cold plate materials.
Document contents
- Data centre cooling and DTC liquid cooling
- Background: copper corrosion and inhibition
- Surface roughness and corrosion
- Objective
- Experimental
- Results: roughness, immersion, electrochemical test, modified ASTM D4340
- Ongoing and future work
- Summary and conclusions
Publication details
- Authors
- Carter Prokesch; Sreya Dutta; Satish Mohapatra
- Publisher
- Dynalene
- Year
- 2026
- Document language
- English
- Source type
- Manufacturer
- Access
- Free to read
- Licence
- Copyright retained; citation only: the publisher’s terms apply to the original document
Original licence note
Official public manufacturer source inspected. No document-specific redistribution permission established; metadata and original brief summaries only. Local downloads are research evidence, not a redistribution package.
Citation
Carter Prokesch; Sreya Dutta; Satish Mohapatra (2026). Influence of Surface Finish on Copper Corrosion in Propylene Glycol-Based Direct-to-Chip Coolants for Data Centers. Dynalene. https://www.dynalene.com/wp-content/uploads/2026/10/SEMITHERM_Dynalene-Sreya-Dutta.pdf
All content and rights belong to the respective authors and publishers. SoSo CAD provides only the citation, its own summary and a link to the source, and is not responsible for the sources' content.