Water chemistry for copper and stainless steel cooling water systems: Corrosion and scaling prevention
The Israel Chemical Society / The Israel Institute of Chemical Engineers · Gilad Kol, Alec Groysman
A 2017 article by Kol and Groysman giving quantitative water chemistry limits for copper (C12200) and 316L stainless steel tubes in 1-30 °C closed-loop cooling water: pH 7.5-8.5 (copper), chloride below 100 and 500 ppm, hardness 60-120 ppm CaCO3.
On this page
Overview
The article addresses closed-loop cooling water systems operating at 1-30 °C that cool computers, control cabinets, server rooms and other heat-emitting applications. The common tube alloys are copper UNS C12200 DHP and stainless steel UNS S31603, but their corrosion resistance depends on adequate control of the water chemistry. The authors note that the literature is scattered and contradictory; the aim is to specify the parameters to monitor, their effect on materials and function, and numeric values for long life. Copper tubes up to 0.30 mm thick and passages as small as 6 mm make perforation and clogging a high risk.
As conditions of use, flow velocity should not exceed 2.5 m/s to avoid erosion-corrosion and stagnation should not exceed 1-2 days, otherwise the system must be emptied, rinsed and dried. The systems are open to air, so dissolved oxygen (about 8 ppm at 25 °C) is present. The article describes general, pitting, crevice, galvanic, erosion, intergranular corrosion and stress-corrosion cracking; copper is susceptible to stress-corrosion cracking with ammonia and stainless steel with chlorides.
The Table 3 recommendations (1-30 °C): pH 7.5-8.5 for copper and 6.0-8.5 for stainless steel; ammonium below 5 ppm for copper; sulfide 0 for copper (mandatory); bicarbonate 70-150 ppm for copper; free CO2 below 15 ppm, aggressive CO2 0; chlorine below 0.2 ppm; suspended solids below 15 ppm; chloride below 100 ppm for copper and 500 ppm for stainless steel; sulfate below 50 ppm for copper; dissolved total iron below 0.2 ppm for copper and 0 for stainless steel; total hardness 60-120 ppm CaCO3; total plate count below 1,000 CFU/ml; sulfate reducing bacteria 0. Except for values marked mandatory, a 10-20% deviation is tolerable.
The article explains the effect of pH using the Pourbaix diagram and discusses hardness, microbiologically induced corrosion (MIC) and monitoring needs. The hardness recommendation is advisory; scale formation depends on many factors and small changes should not be regarded as drastic.
Key points
- Scope: 1-30 °C closed-loop cooling water; copper UNS C12200 DHP and stainless steel UNS S31603 (316L) tubes.
- Flow velocity should not exceed 2.5 m/s; stagnation beyond 1-2 days requires emptying, rinsing and drying.
- pH: 7.5-8.5 for copper; 6.0-8.5 for stainless steel.
- Chloride: below 100 ppm for copper and below 500 ppm for stainless steel; sulfate below 50 ppm for copper.
- Sulfide 0 ppm for copper (mandatory); ammonium below 5 ppm for copper (mandatory); bicarbonate 70-150 ppm for copper.
- Chlorine below 0.2 ppm and suspended solids below 15 ppm; dissolved iron below 0.2 ppm for copper, 0 for stainless steel.
- Total hardness 60-120 ppm CaCO3 is recommended; this is not mandatory.
- Total plate count below 1,000 CFU/ml; sulfate reducing bacteria 0 (mandatory).
- Except for mandatory parameters a 10-20% deviation is tolerable; dissolved oxygen is about 8 ppm at 25 °C.
Using it in design
- Add the Table 3 limits for pH, chloride, sulfate, sulfide, ammonium, hardness and microbiology to the closed-loop water specification according to the tube material (copper or 316L).
- Keep pipe velocity below 2.5 m/s and protect narrow passages (down to 6 mm) from clogging with filters and strainers.
- Define an empty, rinse and dry procedure for commissioning and maintenance stoppages longer than 1-2 days.
- Review solder and weld filler selection for sulfide and ammonia risk (phosphorus-bearing filler metal is attacked by sulfide).
- Set monitoring frequency in operation for pH, conductivity, chloride, total plate count and sulfate reducing bacteria.
Who should read it
Mechanical and corrosion engineers responsible for material selection, water treatment and operation of server room and closed-loop cooling water systems.
Document contents
- Abstract and Introduction
- Cooling Water System Materials
- Conditions of Use
- Common Forms of Corrosion in Cooling Water
- Water Chemistry Requirements (Table 3)
- Effect of Water pH and Electrode Potential on Copper Corrosion
- Water pH Requirements for Stainless Steel
- Sulfide, Ammonia, Bicarbonate and Carbon Dioxide
- Total Hardness
- Total Plate Count and Sulfate Reducing Bacteria
- Conclusion
- References
Publication details
- Authors
- Gilad Kol; Alec Groysman
- Publisher
- The Israel Chemical Society / The Israel Institute of Chemical Engineers
- Year
- 2017
- Document number
- The Israel Chemist and Engineer, Issue 3, pp.12–20
- Document language
- English
- Source type
- Scientific
- Access
- Free to read
- Licence
- Copyright retained; citation only: the publisher’s terms apply to the original document
Original licence note
Publisher PDF downloaded; pp.12–20 inspected selectively. No document-specific commercial redistribution permission established. The URL upload year 2022 is not the June 2017 issue year.
Citation
Gilad Kol; Alec Groysman (2017). Water chemistry for copper and stainless steel cooling water systems: Corrosion and scaling prevention. The Israel Chemical Society / The Israel Institute of Chemical Engineers. The Israel Chemist and Engineer, Issue 3, pp.12–20. https://www.chemistry.org.il/wp-content/uploads/2022/08/ICE_June-2017.pdf
All content and rights belong to the respective authors and publishers. SoSo CAD provides only the citation, its own summary and a link to the source, and is not responsible for the sources' content.